Heat Capacity of Liquid and Solid Polymers at 298 K(1)

Polymer / Heat Capacity (J/mol-K): Cp,solid Cp,liquid
Poly(acrylonitrile), PAN 69.3 -
Poly(Bisphenol A carbonate), PC 300.7 406.9
Poly(1,3-butadiene) 89.5 101.4
Poly(1-butene), PB-1 99.6 118.3
Poly(butyl acrylate) , PBA 211.3 231.0
Poly(butyl methacrylate), PBMA 237.3 263.5
Poly(caprolactam), Nylon 6 165.8 258.3
Poly(caprolactone), PCL 161.5 206.5
Poly(chlorotrifluoroethylene) 101.1 -
Poly(4-chlorostyrene) 141.0 -
Poly(2,6-dimethyl-p-phenylene oxide), PPO 149.4 210.3
Poly(2,6-diphenyl-p-phenylene oxide) 272.8 336.5
Poly(ethyl acrylate), PEA 143.3 180.3
Poly(ethyl methacrylate), PEMA 165.8 203.2
Poly(ethylene glycol), PEG 55.3 91.2
Poly(ethylene terephthalate), PET 219.3 305.4
Poly(ethylene), PE 46.2 62.7
Poly(hexamethylene adipamide), Nylon 6,6 328.3 490.8
Poly(hexamethylene dodecanediamide), Nylon 6,12 482.0 672.3
Poly(hexamethylene sebacamide), Nylon 6,10 448.5 615.6
Poly(isobutene), PIB 93.1 110.1
Poly(isobutyl acrylate) 216.2 230.5
Poly(isobutyl methacrylate) 227.2 273.2
Poly(methacrylic acid), PMAA 112.1 -
Poly(methyl acrylate), PMA 114.0 153.3
Poly(1-methyl-1-butenylene) 108.0 130.3
Poly(methyl methacrylate), PMMA 136.5 182.0
Poly(4-methyl-1-pentene) 141.7 -
Poly(4-methylstyrene) 149.6 197.1
Poly(1-pentene) 116.9 143.1
Poly(propylene), PP 69.0 89.5
Poly(tetrahydrofuran), PTMG, PTHF 116.4 147.9
Poly(thio-1,4-phenylene) 110.2 157.2
Poly(trimethylene glycol) 79.3 119.2
Poly(vinyl acetate), PVA 108.7 162.6
Poly(vinyl alcohol), PVOH 61.5 -
Poly(vinyl benzoate) 164.2 243.1
Poly(vinyl chloride), PVC 62.1 74.1
Poly(α-methylstyrene)  149.7 171.0
Poly[(tetramethylene terephthalate), PBT 267.9 354.5
Poly{[bis(4-chlorophenyl)sulfone]-alt-[bisphenol-A]}, PSU - 678.1
Polyacetal, Poly(methylene oxide), POM 40.2 61.2
Polystyrene, PS 125.7 177.2
Teflon, PTFE 92.6 98.3
(1) The heat capacities are the average of one or more experimental values.